About etching pcbs- I recently enjoyed etching with hardware store=20 muriatic acid and drugstore hydrogen peroxide. when you are done with=20 the solution, neutralize the acid and precipitate the copper with baking=20 soda. Trash the solids and down the drain with the now harmless water. I=20 was using the laser printer on toner transfer paper http://www.pulsarprofx.com/pcbfx/main_site/pages/products/transfer_paper.ht= ml -- I had not much good luck with glossy magazine paper method The etchant: "Mix two parts hydrogen peroxide for every one part=20 hydrochloric acid. When mixed, they form a substance that is a severe=20 skin irritant, and will produce toxic chlorine gas." http://www.wikihow.com/Etch-a-Circuit-Board --=20 Looking forward, Al Shinn --=20 http://www.piclist.com PIC/SX FAQ & list archive View/change your membership options at http://mailman.mit.edu/mailman/listinfo/piclist .